National Aeronautics andSpace Administration Langley Research CenterHampton, Virginia 23681-2199 NASA/CR-2001-211422ICASE Report No. 2001-43 Piezoelectric Polymers J.S. Harrison NASA Langley Research Center, Hampton, Virginia Z. Ounaies ICASE, Hampton, Virginia ICASE NASA Langley Research Center Hampton, Virginia Operated by Universities Space Research Association December 2001 Prepared for Langley Research Centerunder Contract NAS1-97046 PIEZOELECTRIC POLYMERS J. S. HARRISON1 AND Z. OUNAIES2 Abstract. The purpose of this review is to detail the currenttheoreticalunderstandingoftheoriginof piezoelectric and ferroelectric phenomena in polymers; to present thestate-of-the-art in piezoelectric polymers and emergingmaterial systems that exhibit promising properties; and to discuss key characterization methods, fundamentalmodelingapproaches,andapplicationsof piezoelectric polymers. Piezoelectric polymers have been known to exist for more than forty years, but in recent years they have gained notoriety as a valuable class ofsmart materials. Key words. piezoelectricity, amorphous polymers, semicrystalline polymers, ferroelectricity, piezoelectric coefficient, hysteresis, dipole orientation, poling, modeling, piezoelectric characterization Subject classification. Structures and Materials: Materials 1. Introduction. 1.1. Basic Definitions. Upon reviewing the abundance of literature on thesubject,itis clear that there is nostandarddefinitionforsmart materials, and that terms such as intelligent materials, smart materials, adaptive materials, active devices, and smart systems, are often used interchangeably. Theterm smart material generally designates a material that changes one or more of its properties in response to an external stimulus. Themostpopular smart material systems are piezoelectric materials, magnetostrictive materials, shape memoryalloys, electrorheological fluids, electrostrictive materials and optical fibers. Magnetostrictives, electrostrictives, shape memory alloys and electrorheological fluids are used as actuators while optical fibers are used primarily as sensors. Among these active materials, piezoelectric materials are most widelyusedbecause of their wide bandwidth, fast electromechanical response, relatively low power requirements and highgenerativeforces.A classical definition of piezoelectricity, a Greek term for pressure electricity ,is the generation of electrical polarization in a material in response to a mechanical stress. This phenomenon is known as thedirecteffect. Piezoelectric materials also display theconverseeffect;mechanical deformation upon application of electrical chargeorsignal. Piezoelectricity is a property of many non-centrosymmetric ceramics, polymers and other biological systems. A subset of piezoelectricity is pyroelectricity, whereby the polarization is a functionof temperature.Somepyroelectricmaterialsare ferroelectric, although not all ferroelectrics are pyroelectric. Ferroelectricity is a property of certain dielectrics, which exhibit a spontaneous electricpolarization(separationof the center of positive and negative electric charge, makingone side of the crystal positive and the opposite side negative) that can be reversed in direction by the application of an appropriate electric field. Ferroelectricity is named by analogy with ferromagnetism, which occurs in materials such as iron. Traditionally,ferroelectricityis definedforcrystallinematerials, or at least in the crystalline region of semicrystalline materials. In the last couple of years, however, a number of researchershaveexploredthe possibility of ferroelectricity in amorphous polymers, i.e., ferroelectricity without the crystal lattice structure (1). ------ 1 M/S 226, NASA Langley Research Center, Hampton, VA 23681. 2 ICASE,M/S132C, NASA Langley Research Center, Hampton, VA 23681. This research was supported by the National Aeronautics and Space Administration under NASA Contract No. NAS1-97046 while the author was in residence atICASE,NASA Langley Research Center, Hampton, VA 23681-2199. 1 1.2. Characteristics of Piezoelectric Polymers. The properties of polymers are so different in comparison to inorganics (Table 1) that they are uniquely qualifiedto fill niche areas where singlecrystalsandceramicsare incapable of performing as effectively. As noted in Table 1, the piezoelectric strain constant (d 31) for the polymeris lower than that of the ceramic. However, piezoelectric polymers have much higher piezoelectric stress constants (g31)indicatingthatthey are much better sensors than ceramics. Piezoelectric polymericsensors and actuators offer the advantage of processing flexibility because they are lightweight, tough, readily manufactured into large areas, andcanbecut and formed into complex shapes. Polymers also exhibit high strength and high impact resistance (2). Other notable features of polymers are low dielectric constant, low elastic stiffness, and low density,whichresultin a high voltage sensitivity (excellent sensor characteristic), and low acoustic andmechanicalimpedance(crucialfor medical and underwater applications). Polymers also typically possess a high dielectricbreakdownandhigh operating field strength, which means that they can withstand muchhigherdrivingfieldsthanceramics.Polymers offer the ability to pattern electrodes on the film surface, and pole only selected regions. Based on these features, piezoelectric polymers possess their own established area for technicalapplications and useful device configurations. TABLE 1. Property comparison for standard piezoelectric polymer and ceramic materials d31a (pm/V) g31a (mV-m/N)k 31 Salient Features Polyvinylidenefluoride (PVDF)282400.12 flexible, lightweight, low acoustic and mechanical impedance Lead Zirconium Titanate (PZT)175110.34brittle, heavy, toxic a Values shown are absolute values of constants. 2. Structural Requirements for Piezoelectric Polymers. The following sectionsexplain piezoelectric mechanisms for both semicrystallineandamorphouspolymers. Although there are distinct differences, particularly with respect to polarization stability, in the simplest terms, four critical elements exist forallpiezoelectricpolymers , regardlessofmorphology.Assummarized by Broadhurst and Davis (3) these essential elements are: (a) the presenceofpermanentmoleculardipoles;(b) the ability to orient or align the molecular dipoles; (c) the ability to sustainthis dipole alignment once it is achieved; and (d) the ability of the material to undergo large strains when mechanically stressed. 2.1. Semicrystalline Polymers. 2.1.1. Mechanism of piezoelectricity in semicrystalline polymers. In order to render them piezoelectric, semicrystallinepolymers must have a polar crystalline phase. The morphology of such polymers consists of crystallites dispersed within amorphous regions as shown in Figure 1a. The amorphousregion has a glass transition temperature that dictates the mechanical propertiesofthe polymer while the crystallites have a melting temperature that dictates the upper limit of the use temperature. The degree of crystallinity present in such polymers depends on their method of preparation and thermal history. Most semicrystallinepolymers have several polymorphic phases, some of which may be polar. Mechanical orientation, thermal annealingandhighvoltagetreatmenthaveallbeen shown to be effective ininducingcrystalline phase transformations. Stretching the polymer essentially aligns the amorphous strands in the film plane as shown in Figure 1b andfacilitates uniform rotation of the crystallites by an 2 electric field. Depending on whether stretching is uniaxial or biaxial, the electrical and mechanical properties (and therefore the transduction response), are either highly anisotropic or isotropic in the plane of the polymersheet. Electrical poling is accomplished by applying an electric field across the thickness of the polymer as depicted in Figure 1c. An electric field on the order of 50 MV/m is typically sufficient to effect crystalline orientation.Polymer poling can be accomplished using a direct contact method or a corona discharge. The latter method is advantageous since contacting electrodes are not required and large area samples can be poledinacontinuousfashion.This method is used to manufacture commercially available polyvinylidenefluoride(PVDF)film.Someresearchershave alsosuccessfullypoledlargearea polymer films by sandwiching films between polished metal plates under a vacuum. This method essentially eliminates electrical arcing of samples and the need for depositing metalelectrodes on the film surface. Forsemicrystalline polymers the amorphous phase supports the crystal orientation and the polarizationis stable up to the Curie temperature. This polarization can remain constant for many years if it is not influenced by the spurious effects of moisture uptake or elevated temperatures. FIG.1 . Schematic illustration showing random stacks of amorphous and crystal lamellae in PVDF polymer. Figure (1a) represents the morphology after the film is melt cast; (1b) is after orientation of the film by mechanically stretching to several times i ts original length; (1c) is after depositing metal electrodes and poling through the film thickness. 3 2.1.2. Piezoelectric constitutive relationships. The constitutive relations describing the piezoelectric behavior in materials can be derived from thermodynamic principles (4). A tensor notation is adoptedtoidentifythe coupling between the various entities throughthe mechanical and electrical coefficients. The common practice is to label directions as depicted in Figure 2. The stretch direction is denoted as "1". The "2" axis is orthogonal to the stretch direction in the plane of the film. The polarization axis (perpendicular to the surface of the film) is denoted as "3". The shear planes are indicated by the subscripts "4", "5", "6" and are perpendicular to thedirections "1", "2", and "3" respectively. By reducing the tensor elements andusingstandardnotations(5),theresultingequations can be displayed in matrix form as follows 6 5 4 3 2 1 666564636261 565554535251 464544434241 363534333231 262524232221 161514131211 3 2 1 636261 535251 434241 333231 232221 131211 6 5 4 3 2 1 X X X X X X ssssss ssssss ssssss ssssss ssssss ssssss E E E ddd ddd ddd ddd ddd ddd S S S S S S EEEEEE EEEEEE EEEEEE EEEEEE EEEEEE EEEEEE (1) 6 5 4 3 2 1 363534333231 262524232221 161514131211 3 2 1 333231 232221 131211 3 2 1 X X X X X X dddddd dddddd dddddd E E E D D D TTT TTT TTT (2) Piezoelectricity is a cross coupling between the elastic variables, stress X and strain S, and the dielectric variables, electric charge density D and electric field E. It is noted that D is named in analogy to the B-field in ferromagnetism although some authors also refer to it asdielectric or electric displacement. There does not seem to be a standard nomenclature,however, it is the opinion of the authors of this chapter that electric charge density is a better description of this property. The combinations of these variables define the piezoelectric strain constant d, the material compliance s and the permittivity. Other piezoelectric properties are the piezoelectric voltage constant g, stress constant e and strain constant h given by equations in Table 2. For a given constant, the first definition in the table refers to the direct effectwhile the second one refers to the converse effect. The piezoelectric constants are interrelated through the electrical and mechanical properties of the material. Electric field strength and electric 4 charge density are related through the dielectric constant, (where is the permittivity of free space), while stress and strain are related through the compliance according to ijiij gd 0 (3) ijijij dse (4) 2 3 15 6 4 FIG.2 . Tensor directions for defining the constitutive relations The polarization P is a measure of the degree of piezoelectricity in a given material. In a piezoelectric material, a change in polarization P results from an applied stress X or strain S under the conditions of constant temperature and zero electricfield.A linear relationship exists between P and the piezoelectric constants. Due to material anisotropy, P is a vector with three orthogonal components in the 1, 2, and 3 directions. Alternatively, the piezoelectric constants can be defined as jiji XdP (5) jiji SgP (6) The electrical response of a piezoelectric material is a function of theelectrodeconfigurationrelativetothe direction of the applied mechanical stress. For a coefficient, dij, the first subscript is the direction of the electric field or charge displacement while the second subscript gives the direction ofthemechanical deformation or stress. The C2 crystallographic symmetry typical of synthetic oriented,poledpolymerfilm leads to the cancellation of all but five of the dij components (d31, d32, d33, d15 and d24). If the film is poledandbiaxiallyorientedorunoriented, d31= d32 and d15= d24. Most natural biopolymers possess D symmetrywhich yields a matrix possessing only the shear piezoelectricity components d13 and d25. Since the d33 constant is difficult to measure without constraining the 5 sample in its lateral dimension, it is typically determined from Equation 7 whichrelatestheconstantstothe hydrostatic piezoelectric constant, d3h. 3332313 dddd h (7) TABLE 2. Definitions for piezoelectric constants. EquationsUnits d = (dD/dX)E = (dS/dE) X (C/N or m/V) e = (dD/dS)E = -(dX/dE) S (C/m or N/Vm) g = (dE/dX)D = (dS/dD) X (Vm/N or m2/C) h = (dE/dS)D = -(dX/dD) S (V/m or N/C) The electromechanicalcoupling coefficient kij represents the conversion of electrical energy into mechanical energy and vice versa. The electromechanical coupling can be considered as a measure of transduction efficiency and is always less than unity as shown below energyelectricalinput energymechanicaltoconvertedenergyelectrical k 2 (8a) energymechanicalinput energyelectricaltoconvertedenergymechanical k 2 (8b) Some k coefficients can be obtained from measured d-constant as follows TEs d 311 31 31k (9) 2.1.3. Ferroelectricity in semicrystalline polymers. At high electric fields, the polarization that occurs in semicrystallinepolymerssuchas PVDF is nonlinear with the applied electric field. This nonlinearity in polarization is defined as hysteresis. The existence of a spontaneous polarization together with polarization reversal (as illustrated by a hysteresis loop) is generally accepted as proof of ferroelectricity. Figure 3 is an example of the typical hysteresis behavior of PVDF. Two other key properties typically reported for ferroelectric materialsarethe coercive field and theremanentpolarization. The coercive field, Ec, which marks the point where the hysteresis intersectswiththehorizontalaxis,is typically about 50 MV/m at room temperature for many ferroelectric polymers. The remanent polarization, Pr, corresponds to the point where the loop intersects with the vertical axis. The values of Ec and Pr are dependent on the temperature and frequency of measurement. The Curie temperature Tc, is generally 6 lower than but close to the meltingtemperature of the polymer.Below Tc, the polymer is ferroelectric and above Tc, the polymer loses its non-centrosymmetric nature. Althoughferroelectricphenomenonhas been well documented in ceramic crystals, the question of whether polymer crystallites could exhibit dipole switching was debatable for about adecade following the discovery of piezoelectricityinPVDF.Inhomogeneouspolarization through the film thickness which yielded higher polarization on the positive electrode side of the polymerledtospeculations that PVDF was simply a trapped charge electret. These speculations where dispelled when X-ray studies (6) demonstrated that polarization anisotropy vanishes with high poling field strengths and that true ferroelectric dipole reorientation occurs in PVDF. Luongo used infraredto attribute the polarization reversal in PVDF to 180 dipole rotation (7). Scheinbeim has documentedthesameviaXray pole analysis and infrared techniques for odd nylons (8). -80 -60 -40 -20 0 20 40 60 80 -150-100-50050100150 Electric Field(MV/m) P r (mC/m 2 ) Pr Ec FIG. 3. Typical ferroelectric hysteresis loop for PVDF. 2.1.4. State-of-the-art. Pioneering work in the area of piezoelectric polymers by Kawai (9) has led to the development of strong piezoelectric activity in polyvinylidene fluoride (PVDF) anditscopolymerswith trifluoroethylene(TrFE) and tetraflouoroethylene (TFE). These semicrystalline fluoropolymers represent the state of the art in piezoelectric polymersand are currently the only commerciallyavailable piezoelectric polymers. Oddnumbered nylons, the next most widely investigated semicrystallinepiezoelectricpolymers,haveexcellent piezoelectric properties at elevated temperatures but have not yet been embraced in practical application. Other semicrystalline polymers including polyureas, liquid crystallinepolymers, biopolymers and an array of blend combinations have been studied for their piezoelectric potential and are summarized in the followingsection.The chemical repeat unit and piezoelectric constants are depicted in Table 3 for several semicrystalline polymers. 7 TABLE 3. Comparison of piezoelectric properties of some semicrystalline polymeric materials. PolymerStructureT g (oC) Tm (oC) Max Use Temp (oC) d31 (pC/N) Ref. PVDF CCH 2 F F n -351758020-282 PTrFE CCH F F F n 3215090-100122 Nylon-11 NHCH 2 C O 10 n 68195185 3 @ 25oC 14 @ 107oC 22 Polyrurea-9 9CH2 HNCHN O n 50180 - -28 2.1.4.1. Polyvinylidene fluoride (PVDF). Interestintheelectricalproperties of PVDF began in 1969 when Kawai (9) showed that thin films that had been poled exhibited a very large piezoelectric coefficient, 6-7 pCN-1,a value which is about ten times larger than had been observed in any other polymer. As seen in Table 3, PVDF is inherently polar. The spatially symmetrical disposition of thehydrogenandfluorineatomsalongthe polymer chain gives rise to unique polarity effects thatinfluencethe electromechanical response, solubility, dielectric properties, crystal morphology and yield an unusually high dielectric constant.Thedielectricconstantof PVDF is about 12, which is four timesgreaterthanmostpolymers , and makes PVDF attractive for integration into devices as the signal to noise ratio is less for higher dielectric materials.The amorphous phase in PVDF has a glass transition that is well below room temperature (-35C),hencethe material is quite flexible and readily strained at room temperature. PVDF is typically 50 to 60% crystalline depending on thermal and processing history and hasat least four crystal phases ( ,,, and ), of which at least three are polar. The most stable, non-polarphase results upon casting PVDF from the melt and can betransformedintothepolarphase by mechanically stretching 8 at elevated temperatures or into the polarphase by rotating the molecular chain axis with a high electric field (~130 MV/m) (10). The phaseismostimportantfor piezoelectric considerations and has a dipole moment perpendicular to the chain axis of 2.1 D corresponding to a dipoleconcentrationo f7x10 -30 Cm. After poling PVDF,the room temperature polarization stability is excellent, however, polarization and piezoelectricity degrade withincreasing temperature and is erased at its Curie temperature. Previously it was believed that polarization stability was defined only by the melting temperature of the PVDF crystals. Recently, however, some researchers suggest that the polarization stability of PVDF and its copolymersisassociated with Coulomb interactions between injected, trapped charges and oriented dipolesinthe crystals (11). They hypothesize that the thermal decay of the polarization is caused by the thermallyactivatedremoval of the trapped charges from the traps at the surface of the crystals. The role of trapped chargesin stabilizing orientation in both semicrystalline and amorphous polymers is still a subject that needs further study. The electromechanical properties of PVDF have beenwidelyinvestigated. Formoredetails,thereaderisreferredto the wealth of literature that exists on the subjects of the piezoelectric, pyroelectric, and ferroelectric properties (2, 6, 12, 13), and morphology (14-16) of this polymer. 2.1.4.2. Poly(vinylidenefluoride-trifluoroethylene and tetrafluoroethylene) copolymers. Copolymers of polyvinylidene fluoride with trifluoroethylene (TrFE) and tetrafluoroethylene(TFE)havealsobeenshownto exhibit strong piezoelectric, pyroelectric and ferroelectric effects. Here, these polymers are discussed togethersince they behave similarly when copolymerized with PVDF. An attractivemorphologicalfeatureofthecomonomersis that they force the polymer intoanall-transconformation that has a polar crystalline phase, which eliminates the need for mechanical stretching to yield a polar phase. P(VDF-TrFE) crystallizes to a much greater extent than PVDF (up to 90% crystalline) yielding a higher remanent polarization,lower coercive field and much sharper hysteresis loops. TrFE also extends the use temperaturebyabouttwenty degrees, to close to 100oC. Conversely, copolymers with TFE have been shown to exhibitalowerdegreeof crystallinity and a suppressed melting temperature as compared to the PVDF homopolymer. Although the piezoelectric constants for the copolymers are not as large as the homopolymer, the advantages of P(VDF-TrFE) associated with processability, enhanced crystallinity, and higher use temperature make it favorable for applications. Typical values of the piezoelectric constantsforcopolymerswith TrFE are given in Table 3. Recently researchers have reported that highly ordered, lamellarcrystals of P(VDF-TrFE) can be made by annealingthe material at temperatures between the Curie temperature and the melting point. They refer to this material as a "single crystalline film". A relativelylarge single crystal P(VDF-TrFE) 75/25mol%copolymerhas been grown that exhibits a room temperature d33 = -38 pm/V and a coupling factor k33 = 0.33 (17). Zhang et al. (18) have studied the influence of introducingdefectsintothecrystallinestructureofP(VDFTrFE)copolymerusinghigh electron irradiation on electroactive actuation. Extensive structural investigations indicatethattheelectron irradiation disrupts the coherence of polarization domains (all trans chains) and forms localized polar regions (nanometer-sized, all-transchainsinterrupted by trans and gauche bonds). After irradiation, the material exhibits behavior analogous to that of relaxor ferroelectric systems in inorganic materials. The resulting material is no longer piezoelectric but rather exhibits a large electric field-induced strain (5% strain)dueto electrostriction. The basis for such large electrostriction is the large change in the lattice strain as the polymer 9 traverses the ferroelectric to paraelectric phase transition and the expansionandcontraction of the polar regions. Piezoelectricity can be measured in these and other electrostrictives when a DC bias field is applied.Irradiationis typically accomplished in a nitrogen atmosphere at elevated temperatures with irradiation dosages up to 120Mrad. 2.1.5. Other semicrystalline polymers. 2.1.5.1. Polyamides. A low level of piezoelectricity was first reported in polyamides (also known as nylons) by Kawai et al. in 1970 (19). A systematicstudyofodd-numberednylons, however, initiated by the group of Scheinbeim and Newman in 1980 (20), served astheimpetus for more than twenty years of subsequent investigations of the piezoelectric and ferroelectric activity in these polymers. The monomer unit of oddnylons consistsofevennumbersofmethylenegroupsandone amide group with a dipole moment of 3.7D. Polyamides crystallize in all-trans conformations and are packed so as to maximize hydrogen bonding between adjacent amine and carbonyl groups as seen in Figure 4 for an even and an odd numberedpolyamide.Theamidedipolesalign synergistically for the odd-numbered monomer, resulting in a net dipole moment.Theamide dipole cancels for an even-numbered nylon, although remanentpolarizations have been measured for someeven-numberednylonsas discussed later in this chapter. Theunitdipoledensityis dependant on the number of methylene groups present and the polarization increases with decreasing number of methylene groups from 58 mC/m 2 fornylon-11 to 125 mC/m 2 for Nylon-5 (8). Polyamides are known to be hydrophilic. Since the water absorption is associated with hydrogen bonding to the polar amide groups, the hydrophilicityincreases as the density of amide groups increases. Water absorption innylon-11andnylon-7hasbeen shown to be as high as 4.5% (by weight), and more than 12% for nylon-5 (21) while it is less than 0.02% for PVDF and its copolymers. Studies have shown that waterabsorptioncanhavea dramatic effect on the dielectric andpiezoelectric properties of nylons, however, the water does not affect the crystallinityororientationinthermallyannealedfilms(21). Thus, films can be dried to restore their original suite of properties. At room temperature, odd-numbered nylons have lower piezoelectric constants than PVDF, however, when examined above their glass transition temperature, they exhibit comparableferroelectric and piezoelectric properties and much higher thermalstability.Thepiezoelectric d and e constants increase rapidly with temperature. Maximum stable d31 values of 17 pC/N and 14 pC/N are reportedfor Nylon-7 and Nylon-11 respectively. Corresponding values of the electromechanical coupling, k31 are 0.054 and 0.049. Studies have also shown that annealing of nylon films enhances their polarization stability as it promotes more dense packing of the hydrogen bonded sheetstructure in the crystalline regions and hinders the dipole switching due to lowered free volume for rotation (22). Though widely studied, piezoelectric polyamides have not been widelyemployedinapplications.Thisis due in part to its low room temperature piezoelectric response and its problem with moisture uptake. 2.1.5.2. Liquid-crystalline polymers. Liquid crystals consist of highlyorderrodlikeordisklike molecules. At their melting point they partially lose crystalline order, generating a fluid but orderedstate.Theycan formlayered structures called smectic phases or nematic phases with an approximately parallel orientation of the molecular long axis. Meyer (23) was the first topredictthatspontaneouspolarizationcouldbeachievedinliquid crystals based on symmetry arguments. Subsequently, it hasbeenshown that liquid crystalline molecules having 10 chiral carbon atoms linking a mesogenicgroup and end alkyl chains have the possibility of exhibiting ferroelectric behavior in the smectic C phase (SmC*) (24). In this phase the molecular axis tilts from thenormaltothelayer planeandthemoleculardipoles align in the same direction, yielding a net polarization. If such liquid crystalline molecules are introduced into the backbone or as a side group on a polymer,a ferroelectric liquid crystalline polymercanbeobtained.Therearethreerequirements for the appearance of spontaneous polarization in a liquid crystal: a center of chirality; a dipole moment positioned at the chiral center and actingtransversetothemolecular long axis; and the existence of a tilted smectic phase (25). 2.1.5.3. Polyureas. Polyureas are thermosets, long used asinsulators in a number of applications. Until a few years ago, ureas were availablemostlyasinsolublepowders or highly cross-linked resins. In 1987, Takahashi et al. (26) successfully developed a vapor deposition polymerizationmethod and later applied it to the synthesis of polyureas (27). Typically, a vapor depositiontechnique is used by evaporatingOCN-R 1-NH2 and H 2N-R2-NH2 monomers simultaneously on a substrate(whereR 1 and R2 are various aliphatic or aromatic groups). This prevents cross-linking and allows the processing of thicknesses in the hundreds of nanometers to tens of micrometers. Takahashietal.(27) explored the dielectric and pyroelectric properties of polyureas films which led to the discoveryoftheir piezoelectricity. By the early 1990's to the present, various aromatic and aliphatic polyureas were synthesizedandshowntobepiezoelectric(28,29). Aromatic polyureas were the first polyurea structures shown to bepiezoeletric. They exhibit high temperature stability, and have a piezoelectric e-constant of 15 mC/m 2, which remains independent of temperature up to 200C. Their pyroelectric coefficient is high due to their low dielectric loss compared to other polymers. The d-constantisabout5pC/N at room temperature and increases as temperature increases (28). Owingtotheirstructures,aliphaticpolyureaspossess a higher flexibility of their molecular chains. Similarly to polyamides, hydrogen bonds play a large role in stabilizing the orientation polarization that is imparted. Polyureas with odd-numbered methyl groups exhibit an overallnon-zero polarization. Polyurea-9 was first synthesized and processed and an e-constant of 5 mC/m 2 wasreported(28).Polyureas with a smaller number of carbons were then attempted, since it was surmised that it should lead toahigherdensityofureabonddipole. Towards that end, polyurea-5 was synthesized and the e- and d-constants were twice the values of the polyurea-9. Aliphaticpolyureasexhibitaferroelectrichysteresis in addition to being piezoelectric when possessing odd numbers of methyl groups. Their thermal stability and piezoelectric coefficients are highly dependent on the poling temperature (typically 70 to 150C), but lower than those of aromatic polyureas. 11 FIG.4. Schematic depiction of hydrogen-bonded sheets showing dipole directions in the crystal lattices of (a) even (Nylon 4) and (b) odd polyamides (Nylon 5) 2.1.5.4. Biopolymers. Piezoelectricity of biopolymers was first reported for keratin in 1941 (30).Whena bundle of hair was immersed in liquid air, an electric voltage of a few volts was generated between thetipandthe root. When pressure was appliedonthecrosssection of the bundle, an electric voltage was generated. Subsequently piezoelectricity has been observed in a wide range of other biopolymers including collagen (31, 32), polypeptides like poly--methylglutamate and poly--benzyl-L-glutamate(33,34), oriented films of DNA (35), poly-lactic acid (36), and chitin (37). Since mostnaturalbiopolymerspossessD symmetry, they exhibit shear piezoelectricity. A shear stress in the plane of polarization produces electric displacement perpendicular to the plane of the applied stress, resulting in a - d14 = d25 piezoelectric constant. The piezoelectric constants of biopolymersare small relative to synthetic polymers, ranging in valuefrom 0.01 pC/N for DNA to 2.5 pC/Nforcollagen.The electromechanical effect in suchpolymersisattributedto the internal rotation of polar atomic groups linked to 12 asymmetric carbon atoms. Keratin and some polypeptide molecules assume an -helical or a crystallinestructure in which the CONH dipoles align synergistically in the axial direction. Currently, the physiological significance of piezoelectricity in many biopolymers is not well understood, butitisbelievedthatsuchelectromechanical phenomena may have a distinct role in biochemical processes. For example, it is known that electric polarization in bone influences bone growth (38). In one studyapiezoelectric PVDF film was wrapped around the femur of a monkey.Within weeks, a remarkable formation of new bonewas observed. The motion of the animal caused deformation of the film producing a neutralizingioniccurrentinthe surrounding tissue. This minute fluctuating current appears to stimulate the metabolicactivityofbonecellsandto lead to proliferation of bone. 2.2. Amorphous Polymers. The purpose of the following section istoexplain the mechanism and key componentsrequired for developing piezoelectricity in amorphous polymers and to present a summary of polarization and electromechanical properties of amorphous polymers currently under investigation. 2.2.1. Mechanism of piezoelectricity. 2.2.1.1. Dielectric theory. Thepiezoelectricity in amorphous polymers differs from that in semicrystalline polymers and inorganic crystals inthatthepolarization is not in a state of thermal equilibrium, but rather a quasi-stable state due to the freezing-in of molecular dipoles. The result is a piezoelectric-like effect. A theoretical modelforpolymerswithfrozen-indipolarorientation was presented to explain piezoelectricity and pyroelectricity in amorphous polymers such as polyvinyl chloride (39). One of the most important properties of an amorphouspiezoelectricpolymer is its glass transition temperature (temperature below whichthe material exhibits glass-like characteristics, and above which it has rubber-like properties) as it dictates use temperatureand defines the polingprocess conditions. Orientation polarization of molecular dipoles is responsible for piezoelectricity in amorphous polymers. It is induced, as shown in Figure 5, by applying an electric field, Ep at an elevated temperature ( Tp Tg) where the molecular chains are sufficientlymobileandallowdipolealignmentwith the electric field. Partial retention of this orientation is achieved by lowering the temperature below Tg in the presence of Ep, resulting in a piezoelectric-like effect. The remanent polarization, Pr is directly proportional to Ep and the piezoelectric response. Theprocedure used to prepare a piezoelectric amorphous polymer clearly results in both oriented dipoles and space orreal charge injection. The real charges are usually concentratednearthe surface of the polymer, and they are introduced due to the presence of the electrodes. Interestingly, some researchers (40, 41) have shown that the presence of space charges does not have a significant effect on the piezoelectric behavior. The reason is two fold. The magnitude of the space charges is usually not significant with respect to the polarization charges. Secondly, space charges are essentially symmetrical with respect to the thickness of the polymer, therefore, when the material is strained uniformly the contributionto the piezoelectric effect is negligible. 13 TgT p Ep Pr Pr 80 - 100 MV/m tp FIG.5. Poling profile for an amorphous polymer. In what follows, the origins of the dielectriccontributiontothepiezoelectricresponseofamorphous polymers is addressed. The potential energy U of a dipole at an angle with the applied electric field is U= Ecos . Using statistical mechanics and assuming a Boltzman's distribution of the dipoleenergies,themean projection of the dipole moment, <> E, in the direction of the applied electric field is obtained E pE kT kT Ecoth (8) This is the Langevin equation which describes the degree of polarization in a sample when an electric field, E, is applied at temperature T. Experimentally, a poling temperature in the vicinity of Tg is used to maximize dipole motion. The maximum electric field which may be applied, typically 100 MV/m, is determined bythedielectric breakdown strength of the polymer. For amorphous polymers, E / kT ismuchless than one, which places these systems well within the linear region of theLangevinfunction.Theremanentpolarization Pr is simply the polarization during poling minus the electronic and atomic polarizationsthatrelaxatroomtemperatureoncethe field Ep is removed. The following linear equation for the remanent polarization results when the Clausius Mossotti equation is used to relate the dielectric constant to the dipole moment (42) Pr = 0 Ep (9) Itcanbeconcluded that remanent polarization and hence piezoelectric response of a material is determined by , making it a practical criterion to use when designing piezoelectricamorphouspolymers. The dielectric relaxation strength,may be the result of either free or cooperative dipole motion.Dielectric theory yields a mathematical approach for examining the dielectric relaxation due to free rotationofthedipoles,. The equation incorporates Debye's work based on statistical mechanics, the Clausius Mossotti equation, and the Onsagerlocal field, and neglects short range interactions (43) 14 calculated NkT n n 2 0 2 2 2 2 3 2 3 30 20()( () () ) (10) N is the number of dipoles per unitvolume, k is the Boltzman constant, (0) is the static dielectric constant and n is the refractive index. One way to measure Pr for amorphous polymers requires the thermallystimulated current (TSC) method (refer to section on characterization). Pr can be calculated from the liberated charge during TSC, and by reconciling that with the Onsager relation, the dipole density can be calculated: P NEkTr p p 2 2 3 2 3 30 20()( () () ) (11) The piezoelectric constants are related to the polarization. From basic thermodynamics, we have: d Pi i T3 () , (12) Mopsik and Broadhurst (41) have developed a molecular theory of the direct piezoelectric effect inpoled amorphous piezoelectric polymers. In their paper, they found the expression for the hydrostaticcoefficient.Later, this theory was extended and an equation for d31 was obtained (44, 45). Bydifferentiating equation (11) above and modifying it to account for dimensional effects such as in the case of stretching (44, 46) dPS P Sr r311111 1 13 1() () () (13) whereis the Poisson's ratio, is the permittivity at high frequencies, and S11 is the compliance ofthepolymer. The first term accounts for dimensional effects and the second term gives the contribution of the local field effect. 2.2.1.2. Polarizability and polingconditions. Designing an amorphous polymer with a large dielectric relaxation strength and hence piezoelectric response requires the abilityto incorporate highly polar groups at high concentrations and cooperative dipole motion. A studyof the relationship between relaxation times, poling temperaturesandpoling fields is crucial to achieve optimal dipole alignment. Theoretically, the higher the electric field, the better the dipole alignment.The value of the electric field is limited, however, by the dielectric breakdown ofthepolymericmaterial.Inpractice, 100 MV/m is the maximum field that can be applied to these materials. Poling times need to be of the order of the relaxation time of the polymer at the poling temperature. During poling, the temperature is lowered to room temperature while the field is still on, in order to freeze in the dipole alignment. In a semicrystalline material, however, the locking-in of the polarization is supported by the crystalline structure of the polymer, and is therefore stable above the glass transition temperature of the polymer. Sincetheremanent polarization in amorphous polymers is lost in the vicinity of Tg, their use is limited to temperatures well below Tg. This means that the polymersare used in their glassy state, when they are quite stiff thus limiting the ability of the polymer to strain with an applied stress. Thepiezoelectricamorphous polymer may be used at temperatures near its Tg to optimize the mechanical properties, but not too close so as tomaintainthe remanent polarization. 15 Although there is little data addressing the stability of piezoelectric activity in amorphous polymers, it is clear that time, pressure, and temperature can all contributetodipolerelaxationin these polymers. For a given application and use temperature, the effect of these parameters on the stability of the frozen-in dipolealignment should be determined. TABLE 4. Structure, polarization and Tg for piezoelectric amorphous polymers. PolymerStructureT g (C) d31 (pC/N) Pr (mCm2) Reference : PVC n Cl CHCH2 8051644 PAN n C N CHCH2 9022549 PVAc CH O C-CH3O n CH2 30-559 P(VDCNVAc) CH O C-CH3O n C N CHCH2 C N CH2 170105051 PPEN O C N O n 145-1255 (-CN) APB/ ODPA OO N O O O N O O n C N 2205@ 150 C 2059 2.2.2. Examples of amorphous piezoelectric polymers. The literature on amorphous piezoelectric polymers is much more limited than that for semicrystalline systems. This isin part because no amorphous piezoelectricpolymershaveexhibited responses high enough to attract commercial interest. Much of the previous 16 work on amorphous piezoelectric polymers resides in the area of nitrile substituted polymers including polyacrylonitrile (PAN) (47-49), poly(vinylidenecyanide vinylacetate) (PVDCN/VAc) (50-54), polyphenylethernitrile (PPEN) (55, 56) and poly(1-bicyclobutanecarbonitrile) (57). Weakpiezoelectric activity in polyvinyl chloride (PVC) and polyvinyl acetate (PVAc) has alsobeenfound(11,41,58, 59). The most promising of these materials are the vinylidene cyanide copolymers that exhibit large dielectric relaxation strengths and strongpiezoelectricity.Table 4 shows molecular structures of the most commonly encountered amorphous piezoelectric polymers. 2.2.2.1. Polyvinylidene chloride (PVC). Thecarbon-chlorinedipole in polyvinylidene chloride (PVC) has beenorientedtoproducealowlevel of piezoelectricity. The piezoelectric and pyroelectric activities generated in PVC were found to be stable and reproducible. Broadhurst et al. (39) used PVC as a basisforunderstandingand studying piezoelectricity in amorphous polymers. The piezoelectric coefficients d 31 of PVC has been reported in the range of 0.5 to 1.3 pC/N. An improved response was achieved by simultaneous stretching and corona poling of film (44). The enhanced piezoelectric coefficient d31 ranged from 1.5 to 5.0 pC/N. 2.2.2.2. PVDCN-copolymers. In 1980, exceptionally strong piezoelectric activities were found by Miyata et al. (50) for the amorphous copolymer of VDCN and VAc.Thecopolymer was poled at 150-oC (20-oC below its Tg) and cooled to room temperature under the electric field. A Pr = 55 mC/m 2 was obtained for a poling field of 50 MV/m.Thatis comparable to the Pr of PVDF. When local ordering, or paracrystallinity, is inherent in the polymer or is induced by mechanical stretching, an increase in the value of the remanent polarization isobserved.For example,some researchers (51) assert that the large discrepancy between the measured and calculated for PVDCN-VAc may be attributed tolocallyorderedregions in the polymer. For the copolymer PVDCN/VAc, calculated = 30 while measured =125 (51). This large discrepancy in the values of is indicative of cooperative motionofseveral nitrile dipoles within the locally ordered regions of the polymer. Cooperativity means that instead of each dipole acting independently, multiple nitrile dipoles respond to the applied electric field in a unified manner. Althoughtheexistenceofcooperativedipolemotion clearly increases the piezoelectric response of amorphous polymers, the mechanisms by which cooperativity can besystematicallyincorporated into thepolymer structure remain unclear at this time (59). The large relaxation strength exhibited by PVDCN/VAc gives it the largest value of P r and hence d31 of all the amorphous polymers. A number of authors have suggested that PVDCN-VAc alsoexhibitsferroelectric-like behavior(51-53)duetoswitching of the nitrile dipoles under an AC-field. The switching time is long compared to normal ferroelectric polymers. 2.2.2.3. Other VDCN polymers. The homopolymer of vinylidene cyanide is thermally unstable (60) as well as highly sensitive to moisture, but VDCN can be polymerized with a variety of monomers in addition to VAc, such as vinyl benzoate (VBz), methyl methacrylate (MMA) and others forminghighly alternating chains. All of these copolymers show some degree ofpiezoelectricityalthough lower than PVDCN-VAc, which is explained by differentactivationenergies for dipole orientation in the glassy state and different chain mobility depending on the side group. 17 2.2.2.4. Polyacrylonitrile(PAN). Polyacrylonitrile (PAN) is one of the most widely used polymers. Shortly after the PVDCN-VAc system was shown to be piezoelectric, researchers turned their attention to PAN, due to its similarity with the aforementioned polymers. The presence of the large nitrile dipole in PAN indicated that it can be oriented by an applied electric field. PAN presented some challenges not encountered in othernitrilesubstituted polymers however. Although theoretical calculations predicted a strong piezoelectric behavior, it was difficultto pole. Several investigators (47-49) have proposed that the difficulty of poling PAN in the unstretched state is related to the strong dipole-dipole interaction of nitrile groups of the same molecule which repel each other, thuspreventingnormal polarization. Upon stretching, the intermolecular dipole interactions facilitate the packing of the individual chains and give rise to ordered zones. Comstock et al. (47) measuredthe remanent polarization of both unstretched and stretched PAN using the thermally stimulated current method (TSC) and observed a two-fold increaseintheremanent polarization (TSC peak at 90-oC) for PAN that was stretched four times its original length. Another approach is the copolymerization of PAN with another monomer. Researchers have successfully reported a reduction of the hindering effect of the dipole-dipole interactions and an enhancement of the internal mobilityofthe polymersegmentswhenPAN is copolymerized with polystyrene or methylmethacrylate. Berlepsch et al. (49) observedaferroelectric behavior in P(AN-MMA), where, for given temperature and field conditions, a characteristic hysteresis loop is obtained. They concluded that it wasperhapsone rare example where both ferroelectric and frozen-in dipole orientations were superimposed. 2.2.2.5. Nitrile-substituted polyimide. Amorphous polyimides containing polar functional groups have been synthesized (61-63) and investigated for potential use as high temperaturepiezoelectricsensors.(-CN) APB/ODPA, polyimide is one such system. The (-CN) APB/ODPA polyimide possesses the three dipole functionalities shown in Table 5. Typically, the functional groups in amorphouspolymers are pendant to the main chain. The dipoles, however, may also reside within the main chain ofthepolymer, such as the anhydride units in the (-CN) APB/ODPA polyimide. The nitrile dipole ispendanttoaphenylring(=4.2 D), while the two anhydride dipoles (= 2.34 D) are within the chain, resulting in a total dipole moment per repeat unit of 8.8 D. TABLE 5. Values of the dipole moments within the nitrile-substituted polyimide DipolesDipole identity Dipole Moment (Debye) CN Pendant nitrile group 4.18 N O O Main chain dianhydride group 2.34 O Main chain diphenylether group 1.30 18 The remanent polarization Pr of the (-CN)APB/ODPA system by thethermally stimulated current method (TSC) was approximately 20mC/m 2 when poled at 80MV/m for one hour above Tg (64). Excellent thermal stability was observed up to 100C, and no loss of the piezoelectric response was seen afteragingat50C and 100C up to 500 hrs. In an attempt to enhance dipolar orientation and minimizelocalizedarcingduringpoling,partially-cured films of the (-CN)APB/ODPA system were simultaneously corona poled and cured. The alignedpolargroups should be immobilized by additional imidization and subsequent coolinginthe presence of an electric field. Park et al.(64)found that both the Tg and the degree of imidization increased almost linearly with the final cure temperature. The value of Pr appeared to be higher for films cured at lower temperatures. The mobility of the moleculesinapartiallyimidizedstateshouldbehigherthan that of the fully cured one, therefore producing a higher degree of dipole orientation. Theimportanceofdipoleconcentrationon ultimate polarization is evident from a comparison of polyacrilonitrile (PAN) and the polyimide (-CN) APB/ODPA. PAN has a singlenitriledipoleperrepeatunit (=3.5D ) resulting in a dipole concentration of 1.34 x10 28 m-3. This translates into an ultimate polarization of 152 mC/m2 (20). The (-CN)APB/ODPApolyimide,ontheotherhand,has a total dipole moment per monomer of 8.8 D.The dipole concentration of (-CN) APB/ODPA, however, is only 0.136 x 10 28 m -3, resulting in an ultimate polarization of 40 mC/m2, which is less than a fourth of that of PAN. Asaresult,similarpolyimideswithincreased nitrile concentrations were synthesized and characterized. Studies on these polymers show polarization is significantly increased by increasing dipole concentration. Structure-property investigations designed to assess effects of these dipoles on Tg, thermal stability, and overall polarization behavior are currently being pursued. 2.2.2.6. Even numberednylons. Murata et al. (65) have shown that Nylon 6I and 6I/6T exhibits a D-E hysteresis loop over a temperature range of 30 to 65Catafixed maximum field of 168 MV/m. The remanent polarization increased with increasing temperature. It shouldbenotedthatNylon6I and 6I/6T were shown to be completely amorphous. The Pr was about 30 mC/m2. 2.2.2.7. Aliphatic polyurethane. Someresearchers (1) have suggestedthat aliphatic polyurethane systems exhibit ferroelectricity that stems fromthe amorphous part at temperatures above the glass transition temperature. This "liquid state" ferroelectricity is very peculiar, seems to exist, and is supported by the hydrogen bonds present. 3. Characterization and Modeling. 3.1.Characterization. Most piezoelectric characterization methods were developed for crystalline ceramics,andhad to be adapted for piezoelectric polymers. Methods based on resonance analysis and equivalent circuits can be used to characterize semi-crystalline PVDF and its copolymers,asoutlined by IEEE standards (66). Details on applying the resonance analysis to piezoelectric polymers have recently been explored by Sherrit and Bar-Cohen(67).Due to the lossy nature of some polymers, the IEEE standards are not adequate, and other techniques are needed to describe the piezoelectric properties more accurately. 19 Quasi-static direct methods are both versatile and well suited to fullyinvestigate the piezoelectric response ofpolymers. Direct methods of this type are especially appropriate for amorphous polymers. Thermally stimulated current measurements (TSC) (68) are used to measure the remanentpolarizationimparted to a polymer, and direct strain or charge measurements are used to investigate the piezoelectric coefficients with respect to electric field, frequency, and stress. TSC is a valuable tool for characterizing piezoelectric polymers. After poling the polymer, a measure of the currentdissipationandthe remanent polarization as a function temperature can be obtained through the TSC. As the sampleis heated through its glass transition temperature (or Curie temperature in the case of a semicrystalline polymer) at a slow rate(typically1-4oC/min),thedepolarization current is measuredusing an electrometer. The remanentpolarization is equal to the charge per unit area; and is obtained from the data by integrating the current with respect to time and plotting it as a function of temperature: dttiAAQPr )(1 (14) Figure6illustratesa typical TSC result. Since permanent dipoles are essentially immobile at temperatures well below Tg, the current discharge remains low in this temperature range. As temperatureincreasestoandbeyond the Tg, however, the onset of dipole mobility contributes to a significant increase in the currentpeak.Thepeakinthe current and the subsequent polarization maximum usually occurs in the vicinity of the Tg. Directmethodsformeasuringthe strain that results from application of a field, (or vice versa), applying a strain,andmeasuring the accumulated charge, are abundant. To evaluate the piezoelectric strain (converse effect), interferometers, dilatometers, fiber optic sensors, optical levers, linear variable displacement transducers and optical methodsareemployed(69-72).The "out-of-plane" or thickness piezoelectric coefficient, d33, can be ascertained as a function of driving field and frequency. The coefficient is measured based on the equation: SdE33333 (15) where S33 is the strain and E3 is the applied electric field. A modified Rheovibron, or similar techniques, have been used to measure the direct piezoelectric effect, where charges accumulated on the surfaces of the polymer are measured (59). The piezoelectric coefficient, d31, can beobtainedbystraining the polymer along the direction of applied stress with a force F. A charge Q is generated on the surface of the electrodes. A geometric factor is used to produce ageometry independent parameter, i.e., surface charge density per unit applied stress, )/( )/( 31 WtF WLQd (16) which has units of pC/N. W, L and t are the width, length, and thickness of the sample respectively. 20 0 0.005 0.01 0.015 0.02 -5 0 5 10 15 050100150200250 A(mA/m 2 ) P r (mC/m 2) Temperature ( 0C) FIG. 6. Thermally stimulated current plot for typical amorphous poled polymer. PolymerTope lectrodeBottom electrode StressStress StressStress+ + + + FIG.7 . Direct effect in polymers 3.2. Modeling. The methodology for modeling piezoelectric behavior in polymers varies depending on the targeted properties. Approaches cover the range frommacroscale to micro and atomistic scales. A detailed review of computational methods applied to electroactive polymers has been published (73). In some cases, modeling can predict behavior where experiments cannot. Using molecular dynamics, the orientation polarization of the (-CN)APB/ODPApolymerhas been assessed by monitoring the angle,, that the dipolesmakewith an applied electric field (74). The bulk Pr was calculated and the results agreed extremely well with experimental results (61). Computational modeling, however,gaveinsight into the contributions of the various dipoles present in a way experimental results could not. The model predicted that 40% of the orientation polarization wasduetothedianhydride within the backbone of the ODPA monomer, and demonstrated the importance of the flexible ether linkage (oxygen atom) in facilitating dipole alignment. Modeling insight of thiskindisinvaluablein guiding the synthesis of new materials. 21 Modeling of PVDCN-VAc can also play a roleinunderstanding the cooperative motion responsible for the high dielectric relaxation strength of this class of polymers; a fact not possible experimentally (75). Recently, mesoscale simulation was used to describe polarization reversal in PVDF films (76). 4. Applications and FutureConsiderations. The application potential for piezoelectric and other electroactive polymers is immense. To date,ferroelectric polymers have been incorporated into numerous sensing and actuation devices for a wide array of applications. Typical applications include devices in medical instrumentation, robotics, optics, computers, and ultrasonic,underwater and electroacoustic transducers. One important emerging application area forelectroactive polymers is in the biomedical field where polymers are being explored as potential artificial muscle actuators, as invasive medical robots for diagnostics and microsurgery,as actuatorimplantsto stimulate tissue and bone growth, and as sensors to monitor vascular grafts and to prevent blockages (77, 78).Such applications are ideal for polymerssincetheycan be made to be biocompatible and they have excellent conformability and impedance matching to body fluids and humantissue. The intent of this chapter isnottodetailspecificapplicationsbutthe interested reader may refer to excellent sources on applications of piezoelectric and ferroelectric polymers (79-81). In the future, we believe that fertile research areas for piezoelectric polymerswillincludeworktoenhance their properties; to improve their processability for incorporation into devices, and to developmaterialswitha broaderusetemperature range. Fundamental structure-property understanding has enabled the development of numerous semicrystalline and amorphous polymers. Based on this knowledge base, future research which focuses on property enhancement via new chemistries withhigherdipole concentrations and incorporation of dipole cooperativity may yield improved materials. Property enhancements may also be gained fromprocessingstudiesto alterpolymer morphology such as those used to make "single crystalline" fluoropolymers. Development of materials that can operate in extreme environments(high temperature and subambient temperature) is also important for expandingtheutilizationof piezoelectric polymers. Piezoelectric and pyroelectric constants of polymers are considerably lower than for ferroelectric inorganic ceramics. Improvements in properties by incorporating polymers into composites with inorganics to obtain higher electromechanical properties and better mechanical propertiesis also valuable. To date piezoelectric polymer-ceramic composites have been made wherein the polymer serves only as an inactive matrix for the active ceramic phase. This is due to themismatchinpermittivitybetweenthepolymer and ceramic which makes it difficult topolebothphases. Research resulting in active polymer and ceramic phases could yield interesting electromechanical properties. Acknowledgements. The authors wish to express sincere appreciation to Dr. J.A. Young (Lawrence Livermore) for her technical insight in the area of amorphous piezoelectric polymers. The authorswouldalsoliketo thank Suzanne Waltz (NASA Langley) for graphics assistance. 22 REFERENCES [1] T. Y UKI, K. SHIDA, T. KODA, AND S. IKEDA, Polarization Reversal of Aliphatic Polyurethane Above the Glass Transition Temperature, Tenth International Symp. on Electrets, pp. 675-677, 1999. [2] G.T. D AVIS, Piezoelectric and Pyroelectric Polymers. In Polymers for Electronic and Photonic Applications, C.P. Wong,ed., Academic Press, Inc.: Boston, MA, p. 435, 1993. [3] M.G. B ROADHURST AND G.T. DAVIS, in Electrets, G.M. Sessler, ed., Springer-Verlag: New York, NY, Vol. 33, p. 283, 1980. [4] W.P.M ASON, Physical Acoustics and the Properties of Solids, D. Van Nostrand Co. Inc.: Princeton, NJ, 1958. [5] J.F. N YE, Physical Properties of Crystals, Oxford Science Publications, Claredon Press: Oxford, 1957. [6] R.G. K EPLER AND R.A. ANDERSON, Ferroelectricity in Polyvinylidene Fluoride, J. Appl. Phys., 49, No. 3 (1978), pp. 1232-1235. [7] J.P. L UONGO, Far-infrared Spectra of Piezoelectric Polyvinylidene Fluoride , J. Polym. Sci., A-2, 10 (1972), pp. 1119-1123. [8] B.Z. M EI, J.I. SCHIENBEIM, AND B.A. NEWMAN, The Ferroelectric Behavior of Odd-Numbered Nylons , Ferroelectrics, 144 (1993), pp. 51-60. [9] H. K AWAI, The Piezoelectricity of Poly(vinylidene fluoride), Jpn. J. Appl. Phys., 8 (1969), p. 975. [10] K. T ASHIRO, H. TADOKORO, AND M. KOBAYASHI, Structure and Piezoelectricity of Poly(vinylidene fluoride), Ferroelectrics, 32 (1981), p. 167. [11] T. F URUKAWA, Piezoelectricity in Polymers, IEEE Trans. Electr. Insul., 24 (1989), pp. 375-393. [12] G.M. S ESSLER, Piezoelectricity in polyvinylidenefluoride, J. Acoust. Soc. Am., 70, No. 6 (1981), pp. 1596- 1608. [13] A.J. L OVINGER, Ferroelectric Polymers, Science, 220, No. 4602 (1983), pp. 1115-1121. [14] J.B. L ANDO AND W.W. DOLL, The Polymorphism of Poly(vinylidene fluoride). I. The Effect of Head-to-Head Structure, J. Macromol. Sci.-Phys. B2, (1968), p. 205. [15] A.J. L OVINGER, in Developments in Crystalline Polymers, D.C. Basset, ed., Applied Science Publishers: London, UK, Vol. 1, p. 242, 1982. [16] G.T. D AVIS, J.E. MCKINNEY, M.G. BROADHURST, AND S.C. ROTH, Electric-field-induced Phase Changes in Poly(vinylidene fluoride), J. Appl. Phys., 49 (1978), p. 4998. [17] K. O MOTE, H. OHIGASHI, AND K. KOGA, Temperature Dependence of Elastic, Dielectric and Piezoelectric Properties of `Single Crystalline' Films of Vinylidene Fluoride Trifluoroethylene Copolymer , J. Appl. Phys., 81, No. 6 (1997), p. 2760. [18] Q.M. Z HANG, V. BHARTI, AND X. ZHAO, Giant Electrostriction and Relaxor Ferroelectric Behavior in Electron-Irradiated Poly(vinylidene fluoride-trifluoroethylene) Copolymer, Science, 280 (1998), pp. 2101- 2104. [19] H. K AWAI AND I. HENJI, Oyo Buturi, 39 (1970), p. 413. [20] B.A. N EWMAN, P. CHEN, K.D. PAE, AND J.I. SCHEINBEIM, Piezoelectricity in Nylon-11, J. Appl. Phys., 51, No. 10 (1980), pp. 5161-5164. [21] B.A. N EWMAN, K.G. KIM, AND J.I. SCHEINBEIM, The Effects of Water Content on the Piezoelectric Properties of Nylon-11 and Nylon-7, J. Mater. Sci., 25 (1990), pp. 1779-1783. [22] Y. T AKASE, J.W. LEE, J.I. SCHEINBEIM, AND B.A. NEWMAN, High-Temperature Characteristics of Nylon-11 and Nylon-7 Piezoelectrics, Macromolecules, 24 (1991), pp. 6644-6652. 23 [23] R.B. M EYER, L. STRZELECKI, L. LIEBERT, AND P. KELLER, Ferroelectric Liquid Crystals, J. Phys. Lett. (Paris), 36 (1975), p. 69. [24] P. L E BARNY AND J.C. DUBOIS, The Chiral Smectic Liquid Crystal Side Chain Polymers , in Side Chain Liquid Crystal Polymers, C.B. McArdle, ed., Blackie, Chapman and Hall: New York, p. 130, 1989. [25] G. S CHEROWSKY, Ferroelectric Liquid Crystal (FLC) Polymers,in Ferroelectric Polymers, Chemistry, Physics and Application, H.S. Nalwa, ed., Marcel Dekker, Inc.: New York, NY, p. 435, 1995. [26] Y. T AKAHASHI, M. IIJIMA, K. INAGAWA, AND A. ITOH, Synthesis of Aromatic Polyimide Film by Vacuum Deposition Polymerization, J. Vac. Sci. Technol. A, 5 (1987), p. 2253. [27] Y. T AKAHASHI, M. IIJIMA, AND E. FUKADA, Pyroelectricity in Poled Thin Films of Aromatic Polyurea Prepared by Vapor Deposition Polymerization , Jpn. J. Appl. Phys., 28 (1989), p. L408- L410. [28] T. H ATTORI, Y. TAKAHASHI, M. IIJIMA, AND E. FUKADA, Piezoelectric and Ferroelectric Properties of Polyurea-5 Thin Films Prepared by Vapor Deposition Polymerization , J. Appl. Phys., 79 (1996), pp. 1713- 1721. [29] E. F UKADA, History and Recent Progress in Piezoelectric Polymers, IEEE Transactions on Ultrasonics, Ferroelectrics and Frequency Control, 47 (2000), pp. 1277-1290. [30] A.J.P. M ARTIN, Tribo-electricity in Wool and Hair, Proc. Phys. Soc., 53 (1941), p. 183. [31] E. F UKADA, Piezoelectricity and Pyroelectricity of Biopolymers, in Ferroelectric Polymers, Chemistry, Physics and Application, H.S. Nalwa, ed., Marcel Dekker, Inc.: New York, NY, p. 393, 1995. [32] H. M AEDA AND E. FUKADA, Effect of Water on Piezoelectric Dielectric and Elastic Properties of Bone , Biopolymers, 21 (1982), p. 2055. [33] M. D ATE, S. TAKASHITA, AND E. FUKADA, Temperature Variation of Piezoelectric Moduli in Oriented Poly(- methyl-L-glutamate), J. Polymer Sci. A, 2, No. 8 (1970), p. 61. [34] T. F URUKAWA AND E. FUKADA, Piezoelectric Relaxation in Poly(-methyl-L-glutamate), J. Polymer Sci. Polymer Phys., 14 (1976), p. 1979. [35] Y. A NDO AND E. FUKADA, Piezoelectric Properties of Oriented Deoxyribonucleate Films , J. Polymer Sci. Polym Phys., 14 (1976), p. 63. [36] E. F UKADA, Piezoelectric Properties of Poly-L-lactic Acid, Rep. Prog. Polymer Phys., Jpn., 34 (1991), p. 269. [37] Y. A NDO, E. FUKADA, AND M.J. GLIMCHER, Piezoelectricity of Chitin in Lobster Shell and Apodeme, Biorheology, 14 (1977), p. 175. [38] E. F UKADA, Piezoelectricity of Bone and Osteogenesis of Piezoelectric Films, in Mechanisms of Growth Control, R.O. Becker, ed., Charles C. Thomas, Springfield, IL, p. 192, 1981. [39] M.G. B ROADHURST, C.G. MALMBERG, F.I. MOPSIK, AND W.P. HARRIS, Piezo-and Pyroelectricity in Polymer Electrets, Electrets: Charge storage and transport in dielectrics, M.M. Perlman,ed., The Electrochemical Society, Inc., Princeton, NJ, pp.492-504, 1973. [40] M.G. B ROADHURST, W.P. HARRIS, F.I. MOPSIK, AND C.G. MALMBERG, Piezoelectricity, Pyroelectricity and Electrostriction in Polymers, Polymer Preprints, Amer. Chem. Soc. Div., Poly Chem., 14 (1973), p. 820 [41] F.I. M OPSIK AND M.G. BROADHURST, Molecular Dipole Electrets, Journal of Applied Physics, 46 (1975), pp. 4204-4208. [42] B. H ILCZER AND J. MALECKI, Electrets: Studies in Electrical and Electronic Engineering, Vol. 14, Elsevier: New York, NY, p. 19, 1986. [43] H. F ROHLICK, Theory of Dielectrics: Monographs on the Physics and Chemistry of Materials, Vol.42,Oxford: UK, p. 15, 1958. [44] V. B HARTI, T. KAURA, AND R. NATH, Improved Piezoelectricity in Solvent-Cast PVC Films, IEEE Trans. 24 Dielectr. and Electr. Insul., 2, No. 6 (1995). [45] H. S TEFANOU, The Application of a Dipolar Theory to the Piezoelectricity in Vinylidene Fluoride-Cotetrafluoroethylene Polymers, J. Appl. Phys., 50 (March 1979), pp. 1486-1490. [46] R. M EYRUEIX AND O. LEMONNIER, Piezoelectrically Induced Elelctro-optical Effect and Dipole Orientation Measurement in Undoped Amorphous Polymers , Phys. D: Appl. Phys., 27 (1994), pp. 379-386. [47] R.J. C OMSTOCK, S.I. STUPP, AND S.H. CARR, Thermally Stimulated Discharge Currents from Polyacrylonitrile, J. Macromol. Sci.-Phys., B13, No. 1 (1977), pp. 101-115. [48] H. U EDA AND S.H. CARR, Piezoelectricity in Polyacrylonitrile, Polymer Journal, 16 (1984), pp. 661-667. [49] H. VON BERLEPSCH, W. KUNSTLER, A. WEDEL, R. DANZ, AND D. GEIB, Piezoelectric Activity in a Copolymer of Acrylonitrile and Methylacrylate, IEEE Transactions on Electrical Insulation, 24 (1989), pp. 357- 362. [50] S. M IYATA, M. YOSHIKAWA, S.TASAKA, AND M. KO, Piezoelectricity Revealed in the Copolymer of Vinylidenecyanide and Vinylacetate, Polymer J., 12 (1980), pp. 857-860. [51] T. F URUKAWA, M. DATE, K. NAKAJIMA, T. KOSAKA, AND I. SEO, Large Dielectric Relaxations in an Alternate Copolymer of Vinylidene Cyanide and Vinyl Acetate, Japanese Journal of Applied Physics, 25 (1986), pp. 1178-1182. [52] I. S EO, Piezoelectricity of Vinylidene Cyanide Copolymers and their Applications , Ferroelectrics, 171 (1995), pp. 45-55. [53] P.A. M IRAU AND S.A. HEFFNER, Chain Conformatin in Poly(vinylidene cyanide-vinyl acetate): Solid State and Solution 2D and 3D n.m.r. Studies, Polymer, 33 (1992), pp. 1156-1161. [54] M. S AKURAI, Y. OHTA, Y. INOUE, AND R. CHUJO, An Important Factor Generating Piezoelectric Activity of Vinylidene Cyanide Copolymers, Polymer Communications, 32 (1991), pp. 397-399. [55] S. T ASAKA, T. TOYAMA, AND N. INAGAKI, Ferro- and Pyroelectricity in Amorphous Polyphenylethernitrile , Jpn. J. Appl. Phys., 33 (1994), pp. 5838-5844. [56] T. T AKAHASHI, H. KATO, S.P. MA, T. SASAKI, AND K. SAKURAI, Morphology of a Wholly Aromatic Thermoplastic, Poly(ether nitrile), Polymer, 36 (1995), pp. 3803-3808. [57] H.K. H ALL, R.J.H. CHAN, J. OKU, O.R. HUGHES, J. SCHEINBEIM, AND B. NEWMAN, Piezoelectric Activity in Films of Poly(1-bicyclobutanecarbonitrile), Polymer Bulletin, 17 (1987), pp. 135-136. [58] V. B HARTI AND R. NATH, Quantitative Analysis of Piezoelectricity in Simultaneously Stretched and Corona Poled Polyvinyl Chloride Films, Journal of Applied Physics, 82 (1997), pp. 3488-3492. [59] Z. O UNAIES, J.A. YOUNG, AND J.S. HARRISON, An Overview of the Piezoelectric Phenomenon in Amorphous Polymers, Amer. Chem. Society, I.M. Khan and J.S. Harrison, eds., Washington, D.C., 1999. [60] S. T ASAKA, N. INAGAKI, T. OKUTANI, AND S. MIYATA, Structure and Properties of Amorphous Piezoelectric Vinylidene Cyanide Copolymers, Polymer, 30 (1989), pp. 1639-1642. [61] Z. O UNAIES, J.A. YOUNG, J.O. SIMPSON, AND B.L. FARMER, DielectricProperties of Piezoelectric Polyimides, Materials Research Society Proceedings: Materials for Smart Systems II, George et al., eds., Materials Research Society: Pittsburgh, PA, Vol. 459, p. 59, 1997. [62] J.O. S IMPSON, Z. OUNAIES, AND C. FAY, Polarization and Piezoelectric Properties of a Nitrile Substituted Polyimide, Materials Research Society Proceedings: Materials for Smart Systems II, George et al., eds., Materials Research Society: Pittsburgh, PA, Vol. 459 p. 53, 1997. [63] Z. O UNAIES, C. PARK, J.S. HARRISON, J.G. SMITH, AND J. HINKLEY, Structure-Property Study of Piezoelectricity in Polyimides, SPIE Proceedings, Electroactive Polymer Actuators and Devices, Newport Beach, CA, Yoseph Bar-Cohen, ed., Vol. 3369, p. 171, 1999. [64] C.P ARK, Z. OUNAIES, J. SU , J.G. SMITH, JR., AND J.S. HARRISON, Polarization Stability of Amorphous 25 Piezoelectric Polyimides, Materials Research Society Proceedings: Electroactive Polymers,Zhang et al., eds., Vol. 600, 1999. [65] Y. M URATA, K. TSUNASHIMA, AND N. KOIZUMI, Dielectric Hysteresis in some Polyamides, Eighth Symposium on Electrets (ISE 8), pp. 709-714, 1994. [66] IEEE Standard on Piezoelectricity, (IEEE Standard 176-1987), Institute of Electrical and Electronic Engineers, 345 East 47th St., New York, NY 10017, 54 pages. [67] S. S HERRITT AND Y. BAR-COHEN, Electroactive Polymer (EAP) Actuators as Artificial Muscles: Reality, Potential and Challenges, Y. Bar-Cohen, ed., SPIE Press, Bellingham, WA, p. 405, 2001. [68] J. VAN TURNHOUT, Thermally Stimulated Discharge of Polymer Electrets , Polymer Journal, 2 (1971), pp. 173-191. [69] J.T. D AWLEY, G. TEOWEE, B.J.J. ZELINSKI, AND D.R. UHLMANN, Piezoelectric Characterization of Bulk and Thin Film Ferroelectric Materials Using Fiber Optics , MTI Instruments Inc., Application Note. [70] W.Y.P AN, H. WANG AND L.E. CROSS, Laser Interferometer for Studying Phase Delay of Piezoelectric Response, Jpn. J. Appl. Phys., 29 (1990), p. 1570. [71] Q.M. Z HANG, W.Y. PAN AND L. E. CROSS, Laser interferometer for the study of piezoelectric and electrostrictive strains, J. Appl. Phys., 63 (1988), p. 2429. [72] T.L. J ORDAN, Z. OUNAIES, AND T.L. TURNER, Complex Piezoelectric Coefficients of PZT Ceramics: Method for Direct Measurement of d33, Materials Research Society Symposia Proceedings, 459 (1997), p. 231. [73] K.E. W ISE, Electroactive Polymer (EAP) Actuators as Artificial Muscles: Reality, Potential and Challenges , Y. Bar-Cohen, ed., SPIE Press, Bellingham, WA, pp. 267-284, 2001. [74] J.A. Y OUNG, B.L. FARMER, AND J.A. HINKLEY, Molecular Modeling of the Poling of Piezoelectric Polyimides, Polymer, 40 (1999), p. 2787. [75] K.E. W ISE, Structure and Dynamics of P(VDCN-VAc): Insights from Molecular Dynamics , Third SIAM Conference on Mathematical Aspects of Materials Science, May 21-24, 2000, Philadelphia, PA. [76] T. K ODA, K. SHIBASAKI, AND S. IKEDA, Monte Carlo Simulation of Polarization Reversal of Ferroelectric Polymer Polyivinylidene Fluoride, Comp. Theor. Polym. Sci., 10 (2000), pp. 335-343. [77] Y. B AR-COHEN, Electroactive Polymer (EAP) Actuators as Artificial Muscles: Reality, Potential and Challenges, Y. Bar-Cohen, ed., SPIE Press, Bellingham, WA, p. 615, 2001. [78] D. D EROSSI AND P. DARIO, Medical Applications of Piezoelectric Polymers, P.M. Galletti, D.E. DeRossi, and A.S. DeReggi, eds., Gordon and Breach Science Publishers, p. 83, 1988. [79] G.M. G ARNER, The Applications of Ferroelectric Polymers, T. Wang, J. Herbert, and A. Glass, eds., Blackie: London, UK, p. 190, 1988. [80] T.R. M EEKER, The Applications of Ferroelectric Polymers, T. Wang, J. Herbert, and A. Glass, eds., Blackie: London, UK, p. 305, 1988. [81] E. Y AMAKA, The Applications of Ferroelectric Polymers, T. Wang, J. Herbert, and A. Glass, eds., Blackie: London, UK, p. 329, 1988. 26